Effect of Repeated Disinfection Cycles on the Surface Integrity, Color Changes, and Dimensional Stability of Thermoplastic Denture Materials: An Experimental Study
Main Article Content
Abstract
Background: Thermoplastic denture materials such as polyamide and acetal are widely used for flexible and metal-free prostheses, yet they are exposed to daily chemical disinfection that may alter their surface, esthetics and fit. Objective: To evaluate the effect of repeated disinfection cycles on surface roughness and integrity, color change and dimensional stability of two thermoplastic denture materials compared with heat-cured polymethyl methacrylate (PMMA).
Materials and Methods: One hundred twenty disc specimens (n = 40 per material: injection-molded polyamide [PA], injection-molded acetal [AC] and heat-cured PMMA) were allocated to four regimens (distilled water, 0.5% sodium hypochlorite [NaOCl], 2% chlorhexidine gluconate [CHX], and an alkaline peroxide tablet [APT]; n = 10 per subgroup). Each cycle consisted of 10 minutes of immersion; measurements were repeated at baseline and after 30, 90 and 180 cycles. Surface roughness (Ra), scanning electron microscopy (SEM) integrity scores, color difference (ΔE00) and percentage change in diameter were analyzed by two-way ANOVA with Tukey post hoc tests, paired tests with Bonferroni correction, and correlation analysis (α = 0.05).
Results: After 180 cycles all three factors, material, solution and their interaction, significantly affected every outcome (p < 0.001). PA showed the greatest changes: NaOCl and APT raised Ra by about 0.08 µm and produced ΔE00 values of 2.54 and 2.27, whereas the same regimens in PMMA produced ΔE00 of about 1.0 and a diameter change below 0.2%. Diameter change in PA reached 0.53% with NaOCl. Ra gain correlated with ΔE00 (r = 0.76).
Conclusions: Within the limits of this in vitro design, repeated chemical disinfection affected polyamide more than acetal or PMMA, and chlorhexidine was the least aggressive chemical regimen. Material-specific disinfection protocols and periodic surface re-inspection are advisable.